The invention relates to the technical field of the processing of the parts of an oil tank truck, in particular to a method for preparing a coating base solution for the coating of a tank car. First, add 5 sodium pentachlorophenol and 20 water into a container, stirring for 5 minutes; then slowly adding 5 phr of dilute sulfuric acid, stir, add after stirring for 5 minutes; then slowly adding 15 phr acrylic emulsion and 10 parts of water, stir, add after stirring for 5 minutes; and then slowly added 0.3 anthraquinone glycosides, stir, add after stirring for 5 minutes; finally slowly added 0.5 calcium chloride and 15 water, stirring for 15 minutes. Preparation method of base coating liquid of the invention, the method gradually added, can not only improve the solubility between substances, but also avoid the agglomeration of particles may make pretreatment coating liquid foundation had been promoted significantly.
【技术实现步骤摘要】
本专利技术涉及油罐车零部件加工
,具体是涉及一种油罐车罐体涂装用涂装基础液的制备方法。
技术介绍
为了更好的提高油罐车罐体的结构性能,采用先在其表面涂装不溶共络层,然后再涂装色漆。这种加工方法由于在其表面仅涂装不溶共络层,而未采用防护膜衬底,涂装加工后的产品在使用一段时间后,表面的薄膜逐渐的褪去,这样将对油罐车罐体的结构性能产生一定影响,也对产品的品质造成不利后果。
技术实现思路
针对现有技术中存在的技术问题,本专利技术的目的在于提供一种油罐车罐体涂装用涂装基础液的制备方法,为实现上述目的,本专利技术采用了以下技术方案:
一种油罐车罐体涂装用涂装基础液的制备方法,首先向容器中加入5份五氯苯酚钠和20份水,搅拌5分钟;接着缓慢加入5份稀硫酸,边加边搅拌,添加完毕后搅拌5分钟;接着缓慢加入15份丙烯酸酯乳液和10份水,边加边搅拌,添加完毕后搅拌5分钟;然后缓慢加入0.3份蒽醌苷,边加边搅拌,添加完毕后搅拌5分钟;最后缓慢加入0.5份氯化钙和15份水,搅拌15分钟。
本专利技术的有益效果表现在:
1)、涂装方法中使用的涂装基础液,其配方设计合理、新颖,特别是添加了少量的蒽醌苷,可以显著提高涂装基础液的处理效率。通过涂装基础液的配合使用,使油罐车罐体在后续涂装不溶共络层时,不溶共络层的附着力更强,继而提高产品的使用寿命,提升产品的竞争力。
2)、涂装基础液的制备方法,通过逐步添加的方法,不仅能够提高各物质之间的溶解性能,还能避免颗粒团聚的可能,使涂装基础液的预处理能力得到显著的提 ...
【技术保护点】
一种油罐车罐体涂装用涂装基础液的制备方法,其特征在于首先向容器中加入5份五氯苯酚钠和20份水,搅拌5分钟;接着缓慢加入5份稀硫酸,边加边搅拌,添加完毕后搅拌5分钟;接着缓慢加入15份丙烯酸酯乳液和10份水,边加边搅拌,添加完毕后搅拌5分钟;然后缓慢加入0.3份蒽醌苷,边加边搅拌,添加完毕后搅拌5分钟;最后缓慢加入0.5份氯化钙和15份水,搅拌15分钟。
【技术特征摘要】
1.一种油罐车罐体涂装用涂装基础液的制备方法,其特征在于首先向容器中加入5份五氯苯酚钠和20份水,搅拌5分钟;接着缓慢加入5份稀硫酸,边加边搅拌,添加完毕后搅拌5分钟;接着缓慢加入15份...